Strength Of A Brazed Joint Under Pressure?

Potatoes last one shot, so build reusable! Discuss ammo designs and ideas. Tough to find cannon part or questions? Ask here!
User avatar
ramses
Staff Sergeant 2
Staff Sergeant 2
United States of America
Posts: 1679
Joined: Thu May 29, 2008 6:50 pm

Thu Apr 05, 2012 8:09 pm

FighterAce wrote:So what would be the preferred method for joining a 15mm OD, 1.6mm wall drawn Cu pipe with a thread to pipe fitting? Operating pressure around 800psi.
Honestly, I would say solder it. If the joint is .25" long (conservative), that gives you .4638 sq in of shear area. The shear strength of 50/50 lead tin solder is 5220 PSi, so the strength of the joint would be 2421 lbs.

The cross section area in this case is .678 in, so your fail pressure is 3570 PSI. This gives you a safety factor of 4.4. (Check my calculations anyway)

If this is for a barrel, it will never see the full working pressure along its axis; there is nowhere for the pressure to act to pull the joint apart except from projectile friction.
POLAND_SPUD wrote:even if there was no link I'd know it's a bot because of female name :D
User avatar
FighterAce
Specialist 2
Specialist 2
Croatia
Posts: 295
Joined: Fri Oct 23, 2009 1:28 pm
Location: Croatia/Zagreb
Has thanked: 1 time
Been thanked: 4 times
Contact:

Thu Apr 05, 2012 8:25 pm

Holy smokes... those numbers are good. Even more so since the joint is .5" long. I thought soft solder wouldn't work for such pressures but I'm glad I was wrong. Its actually for a two stage HP pump. Thanks ramses!
“The combined synergy of a man and rifle is matchless.
The steadiness of hand, the acuity of vision and finally
the art of knowing how to make the rifle an extension of the
body all equate to the ultimate synthesis of man and machine.”
User avatar
Technician1002
Captain
Captain
Posts: 5189
Joined: Sat Apr 04, 2009 11:10 am

Thu Apr 05, 2012 11:03 pm

The problem with lead tin solder is mechanical fatigue. If the joint is subject to repeated stresses mechanically the solder is known for cracking type failures.

In electronics, this is referred to as a cold solder joint. Mechanical stress on components such as volume controls and headphone jacks are a common failure. Another common failure point is power transistors and resistors where they see thermal cycles from heating and cooling. Below is what one of these intermittent thermal failures looks like. A soldered copper barrel may come unsolderd from mechanical fatigue.
Image
User avatar
Crna Legija
First Sergeant 2
First Sergeant 2
Posts: 2333
Joined: Sun Jul 20, 2008 5:14 am
Location: australia

Thu Apr 05, 2012 11:19 pm

Technician1002 wrote:The problem with lead tin solder is mechanical fatigue. If the joint is subject to repeated stresses mechanically the solder is known for cracking type failures.
that happened to my ps3 it just stopped reading CD's all a sudden and i search on the web lots of people turn it on and wraped it in a blanked to let it get hot and re solder the bad peace, I didn't think it would work but sure enough it did left it for a hour in a blanket in my back yard then let it cool off and it works again just fine.
'' To alcohol... The cause of, and solution to, all of life's problems.”
--Homer Simpson

Add me on ps3: wannafuk, 8/11/11 cant wait
User avatar
Gun Freak
Lieutenant 5
Lieutenant 5
Posts: 4971
Joined: Mon Jan 25, 2010 4:38 pm
Location: Florida
Been thanked: 8 times

Fri Apr 06, 2012 9:25 am

Haha that's awesome Crna :D

Tech, would the same concept apply to soldered copper chambers?
OG Anti-Hybrid
One man's trash is a true Spudder's treasure!
Golf Ball Cannon "Superna"M16 BBMGPengunHammer Valve Airsoft SniperHigh Pressure .22 Coax
Holy Shat!
User avatar
jhalek90
Specialist 4
Specialist 4
Posts: 498
Joined: Fri Aug 14, 2009 5:37 pm

Fri Apr 06, 2012 10:52 am

Little bit of info on brazing, if done correctly, brazing can be stronger than the metal you are brazing.


I did brazing of stainless steel, brass, titanium, and aluminum for about 3 years as a job, every once and a while are parts would be tested in all sorts of fun ways, the SS brazing were able to withstand over 20,000lbs of sheer force, which eventually snapped the SS like a rubber band that you pulled to hard.

Some of our joints were pressure tested as well, i've never had one fail, even at 10,000psi hydraulic pressure.

Brazing, is alot stronger then solder, but requires a little bit of research as to proper filler material (solder?) and flux, as well as temperature.

Most of the stuff i brazed was SS and titanium. Most of the joins were about 1/4'' to 1/2'' and where done at a rather particular temp range.
To hot and you fatigue the metal, to cold and you don't get as strong of a joint as you could.

if you are going to "solder" copper, you should be fine, as long as you make sure your joints are fully soldered, but don't get them to warm.

For copper i use a propane torch, just head the copper, near the join, and let the solder wick into the joint, with the right flux, this is relatively easy.

If anyone is interested, i worked here: http://www.thompsonsurgical.com/
WARNING! the home page has photos of surgery, and is not the the weak stomached.
jackssmirkingrevenge wrote:I wonder... if you put flammable vapours inside a lady... could you get her to diesel?
POLAND_SPUD wrote:Anything is possible with the proper 3-way valve.
User avatar
cammyd32
Specialist 3
Specialist 3
Great Britain
Posts: 326
Joined: Fri Apr 29, 2011 7:00 am

Fri Apr 06, 2012 11:42 am

Some of our joints were pressure tested as well, i've never had one fail, even at 10,000psi hydraulic pressure.

Sheesh! well I think that these joints I'm going to make are going to be perfectly adequate bearing in mind I'm working at 250 psi!
after long hours into the night sourcing parts I've decided on aluminium as a base material seeing as it will come out cheaper, and for some reason only in aluminium can I actually find the pipe bores that I need!
So I'm wondering.. aluminium for pressure? any links to aluminium cannons on the site would be warmly received, and thanks all for the advice!
Goats spudz
Specialist 4
Specialist 4
Posts: 458
Joined: Tue Aug 02, 2011 12:31 pm
Contact:

Fri Apr 06, 2012 11:47 am

if your using steel just weld it, i mig welded a hydraulic fitting to my fridge compressor and it has taken 1000 psi easily. also they make 4500 psi air bottles from aluminium.
Where's my Chuck key?
User avatar
Crna Legija
First Sergeant 2
First Sergeant 2
Posts: 2333
Joined: Sun Jul 20, 2008 5:14 am
Location: australia

Fri Apr 06, 2012 6:55 pm

Goats spudz wrote:if your using steel just weld it, i mig welded a hydraulic fitting to my fridge compressor and it has taken 1000 psi easily. also they make 4500 psi air bottles from aluminium.
Image
'' To alcohol... The cause of, and solution to, all of life's problems.”
--Homer Simpson

Add me on ps3: wannafuk, 8/11/11 cant wait
User avatar
cammyd32
Specialist 3
Specialist 3
Great Britain
Posts: 326
Joined: Fri Apr 29, 2011 7:00 am

Sun Apr 08, 2012 6:32 am

Crna Legija wrote:
Goats spudz wrote:if your using steel just weld it, i mig welded a hydraulic fitting to my fridge compressor and it has taken 1000 psi easily. also they make 4500 psi air bottles from aluminium.
Image
haha, love it! :D
User avatar
al-xg
Corporal 2
Corporal 2
Great Britain
Posts: 643
Joined: Fri Jan 19, 2007 12:29 pm

Sun Apr 08, 2012 8:15 am

There are many grades of aluminium out there, the weakest grades having a tensile strength nearly 10 times lower than the higher end stuff.
Goats spudz
Specialist 4
Specialist 4
Posts: 458
Joined: Tue Aug 02, 2011 12:31 pm
Contact:

Sun Apr 08, 2012 12:47 pm

Crna Legija wrote:
Goats spudz wrote:if your using steel just weld it, i mig welded a hydraulic fitting to my fridge compressor and it has taken 1000 psi easily. also they make 4500 psi air bottles from aluminium.
Image
http://www.luxfer.net/products/paintbal ... =undefined silly person go crawl back under your rock.
Where's my Chuck key?
User avatar
cammyd32
Specialist 3
Specialist 3
Great Britain
Posts: 326
Joined: Fri Apr 29, 2011 7:00 am

Sun Apr 08, 2012 12:58 pm

There are many grades of aluminium out there, the weakest grades having a tensile strength nearly 10 times lower than the higher end stuff.
If you want specifics I'm talking about standard t6 grade aluminium, about a 1.7 mm wall and 32mm in external diameter.
Goats spudz
Specialist 4
Specialist 4
Posts: 458
Joined: Tue Aug 02, 2011 12:31 pm
Contact:

Sun Apr 08, 2012 1:02 pm

if you tig weld it then it will work :D
Where's my Chuck key?
User avatar
ramses
Staff Sergeant 2
Staff Sergeant 2
United States of America
Posts: 1679
Joined: Thu May 29, 2008 6:50 pm

Sun Apr 08, 2012 1:30 pm

Keep in mind that TIG welding aluminum reduces the surrounding area to the T0 condition, and that you can't really heat treat it yourself.
POLAND_SPUD wrote:even if there was no link I'd know it's a bot because of female name :D
Post Reply